Eight common flexo print defects what causes them, and how to correct them on press.

This guide sets out the eight print defects our technical team is called out to most often. Each entry describes what the defect looks like on the printed web, lists the probable causes in the order worth checking them, and gives the corrective action.  

If you still have questions our technical service team supports customers across Europe, the Middle East and Africa directly on site. 

Before you change anything: work the variables in order

Changing three settings at once tells you nothing about which one fixed the problem. When a defect appears mid-run, isolate it in this sequence:

  1. The ink. Check viscosity against the job standard first. Then check solvent balance and the condition of the ink, contamination and how long the ink has been circulating.
  2. The transfer. Anilox cell volume and condition, doctor blade type, angle and pressure, printing plate inspection for manufacturing defects or surface wear, verification of plate hardness and relief depth. Mounting tape, type and hardness.  
  3. The machine. Impression settings between plate cylinder, anilox and substrate; web tension; dryer performance; chill drum function.
  4. The substrate. Corona treatment level and age of the film, surface cleanliness, thickness tolerance, wetting behaviour. 

Potential Issues

What you see:

The ink does not adhere sufficiently to the substrate and can be removed easily,  typically failing a tape test.

Adhesion failures are the most commercially serious defect on this list, because they often pass visual inspection at the press and are only discovered downstream at lamination, filling or in the customer's hands. Treat surface energy and ink system compatibility as your first two checks. 

lack of ink adhesion with error
With Error
lack of ink adhesion correct image
Without Error

Start here:

Measure the film's surface tension before adjusting anything on the press. Corona treatment decays with time in storage, and an under-treated or aged film will defeat every other correction you make.

Potential issues & solutions

Potential issue
Insufficient corona treatment on the film
Recommended solution

Evaluate the film's treatment level. Adjust the machine's refreshing treatment and consider using film with enhanced treatment

Potential issue
Ink drying is inadequate
Recommended solution

Incorporate faster drying solvents and/or increase the air circulation and heat supply

Potential issue
Film contamination due to surface impurities
Recommended solution

Before printing, apply a suitable primer, or alternatively switch to a film batch with better surface properties

Potential issue
Ink viscosity is excessively low
Recommended solution

Elevate the ink's viscosity by adding fresh ink

Potential issue
Accumulation of multiple colour layers
Recommended solution

Confirm that the initial ink layer exhibits strong adhesion and resists dissolution by subsequent ink applications

Potential issue
The printing material is not compatible with the ink
Recommended solution

Verify that the appropriate ink system for the specific material is being used

What you see:

The ink adheres to the reverse side of the film and causes damage when the substrate is unwound.

Blocking is a heat-and-solvent problem. It is nearly always the result of ink that has not fully released its solvent before the web is wound, or of a reel that is wound too tightly, too warm, or both. 

blocking with error image
With Error
blocking correct image
Without Error

Start here:

Measure the web temperature at the winder. If the film is going into the reel warm, no adjustment to the ink will solve the problem.

Potential issues & solutions

Potential issue
Excessive retarder present in the ink
Recommended solution

Exchange the current ink

Potential issue
Film temperature at the winder is excessively high
Recommended solution

Decrease the tunnel dryer's temperature and verify the cooling cylinder functionality

Potential issue
Inadequate pretreatment level of the film
Recommended solution

Check the pretreatment and the age of the film. Use the inline corona treatment (refresh)

Potential issue
Ink drying process is too slow
Recommended solution

Enhance the dryer's performance. Employ a faster drying solvent. Decrease the printing speed

Potential issue
Ink volume transferred is excessively high
Recommended solution

Choose anilox rollers designed for a lower transfer volume

Potential issue
Ink viscosity is too high
Recommended solution

Lower the ink viscosity by incorporating solvents

Potential issue
The cooling system of the web is malfunctioning
Recommended solution

Get in touch with the service department

Potential issue
Winding tension at the winder is excessive
Recommended solution

Decrease the winding tension

What you see:

Very faint images of the design appearing in solid areas of the print. The defect shows up when a solid background carries negative elements — reversed text, windows, cut-outs.

Ghosting is an ink starvation phenomenon. The anilox cannot deliver enough ink to the solid area immediately following the negative element, and the shortfall reproduces as a faint echo of the shape that caused it.

ghost effect with error
With Error
ghost effect correct image
Without Error

Start here:

Inspect the anilox for cell blockage before changing the ink. A partially plugged roll starves the plate in exactly the pattern that produces ghosting. 

Potential issues & solutions

Potential issue
Insufficient ink in anilox cells (ink starvation)
Recommended solution

Opt for a higher volume anilox; increase the pressure in the chamber/doctor blade; ensure an adequate ink level

Potential issue
Ink drying within the cells, leading to blocked flow
Recommended solution

Incorporate retarders; switch to a slower drying solvent ink; regulate temperature and humidity levels

Potential issue
Problems with the doctor blade, such as misalignment or an incorrect blade type
Recommended solution

Optimise the blade type, angle and pressure; ensure the chamber is properly aligned, use a 3 blade system

Potential issue
Dirty or worn anilox roll, resulting in poor cell fill or release
Recommended solution

Regularly clean, recondition or re-engrave the anilox roll

What you see:

Small areas where ink has pulled back from the substrate, leaving unprinted or light points within a solid.

Pinholes are a wetting failure. The ink is being applied but will not hold as a continuous film  either because the surface rejects it, or because the ink film is too thin to level.

pinholes with error image
With Error
pinholes correct image
Without Error

Start here:

Use the correct hardness tape and increase the printing pressure and the ink film thickness. if you are running water-based inks, check pH first. It drifts steadily through a long run and takes wetting behavior with it. 

Potential issues & solutions

Potential issue
The hardness of the plate is high
Recommended solution

Use a softer plate

Potential issue
The hardness of the tape is low
Recommended solution

Use a harder tape

Potential issue
The film or printing plate surface is irregular
Recommended solution

Increase the pressure setting, or replace the film or printing plate

Potential issue
The substrate exhibits inconsistent wetting
Recommended solution

Utilise more suitable printing material, or increase the ink layer thickness by raising viscosity or by using a higher volume anilox roller

Potential issue
The ink is foaming
Recommended solution

Introduce a defoaming agent

Potential issue
The pH level of water-based inks is too low
Recommended solution

Perform a pH value adjustment

What you see:

A thin outline or halo around printed images, screen dots or text, usually denser than the main image.

The halo is squeezed ink. Excess pressure or excess volume forces ink out beyond the edge of the printing element, where it deposits as a ring. It is almost always a pressure and volume problem, not an ink problem. 

halo effect with error image
With Error
halo effect correct image
Without Error

Potential issues & solutions

Potential issue
Plate cylinder is out of round
Recommended solution

Check plate cylinder eccentricity

Potential issue
The anilox roller's transferred volume is excessively high
Recommended solution

Choose an anilox roller that provides a lower transferred volume

Potential issue
Excessive pressure setting between the plate cylinder and the substrate
Recommended solution

Reduce the pressure setting

Potential issue
The pressure within the chamber doctor blade system is too low
Recommended solution

Increase the pressure within the chamber doctor blade system

Potential issue
The pressure setting between the anilox roller and the plate cylinder is too high
Recommended solution

Reduce the pressure setting

What you see:

A mottled or marbled appearance across solid print areas — the ink layer is visibly uneven rather than flat.

Mottling points to inconsistent ink transfer or an uneven contact surface. Work through the plate, then the ink body, then the substrate. 

ink mottling with error image
With Error
ink mottling correct image
Without Error

Potential issues & solutions

Potential issue
The printing plate surface is cloudy/uneven or shows visible damage
Recommended solution

Produce a new printing plate

Potential issue
The ink's viscosity is excessively low
Recommended solution

Add fresh ink and/or an ink blend to achieve the appropriate resulting viscosity

Potential issue
Presence of foreign bodies or impurities on the plate cylinder
Recommended solution

Carefully clean the plate cylinder

Potential issue
The substrate surface is uneven
Recommended solution

Employ softer printing plates

Potential issue
The film surface is contaminated
Recommended solution

Filter the ink or use fresh ink

Potential issue
The ink viscosity is too high
Recommended solution

Incorporate solvent into the ink

Potential issue
The doctor blade pressure is either too high or too low
Recommended solution

Adjust the doctor blade pressure as required

What you see:

Ink connections forming between individual screen dots on the printing plate. The depressions between dots fill with ink and the halftone closes up.

Bridging is a drying-speed and viscosity problem. The ink is becoming too tacky on the plate before it transfers, or there is simply too much of it for the screen ruling being run. 

dot bridging with error image
With Error
dot bridging correct image
Without Error

Potential issues & solutions

Potential issue
Ink drying speed is excessively fast
Recommended solution

Decrease the ink's evaporation rate by incorporating a retarder solvent

Potential issue
Ink viscosity is excessively high
Recommended solution

Adjust the ink's viscosity to the optimal level

Potential issue
Anilox roll has high volume and few lines relative to the plate lines
Recommended solution

Replace the anilox roll with one that has more lines and less volume

Potential issue
Presence of contaminants within the ink
Recommended solution

If impurities are found in the ink, it must be replaced or filtered

Potential issue
Imbalance in the ink solvent mixture
Recommended solution

Adjust the ink's drying speed. Modify the solvent mixture. Enhance the dryer's performance between the printing units.

What you see:

Excessive dot gain on the substrate, reducing detail and flattening contrast across the image.

Some dot gain is inherent to flexography and is compensated for in prepress. The defect is gain beyond what the curve accounts for  which is a mechanical problem, not a design one.

dot gain with error
With Error
dot gain correct image
Without Error

Potential issues & solutions

Potential issue
Excessive thickness variation in the printing plate or double-sided adhesive tape
Recommended solution

Replace the printing plate or the double-sided adhesive tape

Potential issue
The printing plate is overly soft, or the double-sided adhesive tape is too rigid
Recommended solution

Use a harder plate or/and softer tape

Potential issue
The pressure setting between the plate cylinder and the substrate is too high
Recommended solution

Decrease the pressure setting

Potential issue
The film's thickness tolerance is too large
Recommended solution

Reduce the plate cylinder's pressure, or replace the film

Potential issue
Incorrect calculation of dot gain
Recommended solution

Adjust the dot gain curve accordingly

Potential issue
The central drum's temperature is either too high or too low
Recommended solution

Contact the maintenance department to fix the issue

Our technical support is here to help

DF Inks’ technical service team works on site with converters across Europe, the Middle East and Africa, supported by our own laboratories and production facilities in Greece, Romania and Nigeria. We formulate the ink, so we can customize it for converters not just recommend a workaround.

FAQs about flexographic printing defects

The most common causes are insufficient corona treatment on the film, an ink system that does not match the substrate, inadequate drying, and surface contamination. Check the film's treatment level first, corona treatment decays during storage, and an aged film will fail a tape test regardless of ink performance.

Ink mottling comes from uneven ink transfer. Check the plate surface for damage or clouding, then ink viscosity in both directions, too low and too high both produce it, then contamination on film, and finally doctor blade pressure.

Many can be corrected in-run, particularly viscosity, doctor blade pressure and dryer settings. Defects rooted in the plate, anilox condition or substrate batch require a stop. Change one variable at a time and record the result, simultaneous adjustments make the cause impossible to identify.