Eight common roto print defects, what causes them, and how to correct them on press.
This guide sets out the eight print defects our technical team is called out to most often in rotogravure production. Each entry describes what the defect looks like on the printed web, lists the probable causes in the order worth checking them, and gives the corrective action.
If you still have questions our technical service team supports customers across Europe, the Middle East and Africa directly on site.
Before you change anything: work the variables in order
Changing three settings at once tells you nothing about which one fixed the problem. When a defect appears mid-run, isolate it in this sequence:
- The ink. Check viscosity against the job standard first. Then check solvent balance and drying speed, resolubility, contamination, and how long the ink has been circulating. Confirm the ink system matches the substrate and the application.
- The transfer. Cylinder cell depth and geometry, chrome quality and surface condition, cylinder balance and concentricity. Doctor blade type, angle, pressure, parallelism, cleanliness and blade support.
- The machine. Impression roller pressure and durometer; web tension through printing and rewind; oven temperature and air velocity; chill roll function and temperature relative to the dew point; electrostatic assist.
- The substrate. Corona treatment level and age of the film, surface cleanliness, thickness tolerance, temperature on entry to the press, wetting behaviour.
Record what you changed and what happened. A defect log turns one operator's fix into plant-wide knowledge.
Potential Issues
What you see:
The ink does not adhere sufficiently to the substrate and can be removed easily, typically failing the tape adhesive resistance test.
Adhesion failures are the most commercially serious defect on this list, because they often pass visual inspection at the press and are only discovered downstream after lamination, filling or in the customer's hands. Treat ink system compatibility and surface energy as your first two checks.
Start here:
Μeasure the film's surface tension before adjusting anything on the press. Corona treatment decays with time in storage, and an under-treated or aged film will defeat every other correction you make.
Potential issues & solutions
What you see:
Τhe ink adheres to the reverse side of the film and causes damage when the substrate is unrolled.
Blocking is a heat-and-solvent problem. It is nearly always the result of ink that has not fully released its solvent before the web is wound, or of a reel that is wound too tightly, too warm, or both.
Start here:
Μeasure the web temperature at the rewind. If the film is going into the reel warm, no adjustment to the ink will solve the problem.
Potential issues & solutions
What you see:
Α visible ink mist in non printing areas, which also leads to an increased colour density in the unprinting areas.
Hazing is a doctor blade and cylinder surface problem. Ink that should have been wiped clear of the cylinder land areas is carried through to the substrate, so look at how the blade is meeting the cylinder before you look at the ink.
Start here:
Check the blade setting and parallelism across the full cylinder width. Note that both a rough cylinder and an over polished one cause hazing, so confirm the surface condition before deciding to polish.
Potential issues & solutions
What you see:
Relatively short stripes that appear and disappear randomly on the printed web.
Comets are caused by something passing under the doctor blade. A particle, a nick in the cylinder or a flaw in the blade lifts it momentarily and the ink escapes as a short tail. Because the cause travels, the defect appears and vanishes rather than holding a fixed position.
Start here:
Filter the ink and clean the blade before touching the cylinder. Most comets are debris, and polishing a cylinder that was never the problem costs you a cylinder.
Potential issues & solutions
What you see:
Ink bleeds from the printed area into the unprinted area.
Bleeding is a trapping problem between colours. The first ink down has not dried enough to accept the next, so the second colour redissolves it and carries it beyond the printed edge. Work on the drying of the first station before you touch the second.
Start here:
Confirm the first colour is fully dry before the web reaches the next station. Raise web temperature and air velocity at that station first, and only then adjust the solvent blend of the following colour.
Potential issues & solutions
What you see:
A dotted or marbled printed image across the solid printing area, with weak ink strength and grainy large format printing.
Mottling points to inconsistent ink transfer out of the cells. Viscosity is the usual cause and it fails in both directions, so measure it rather than assuming which way it has drifted.
Start here:
Measure viscosity against the job standard rather than adjusting by eye. If the ink or the substrate has come straight from a cold store, let both reach room temperature before you judge anything else.
Potential issues & solutions
What you see:
The ink is drying inside the cylinder cells, so the cells no longer fill or release correctly and the print weakens or breaks up.
This is a drying-speed problem at the cylinder rather than in the oven. The ink is losing solvent before it reaches the substrate, either because it is formulated too fast, or because air movement around the station is accelerating evaporation.
Start here:
Look for air movement across the station before changing the ink. A dryer exhausting towards the cylinder, or an open door, will dry cells faster than any solvent adjustment can compensate for.
Potential issues & solutions
What you see:
Ink is picked up off the web by the next printing cylinder, removing it from the printed image.
Picking means the ink is still wet when it reaches the following station or the next roll. It is the same root cause as bleeding but shows as removal rather than spread, and the fix sits in drying capacity and web temperature.
Start here:
Check the idler rolls before adjusting the ink. A tacky roll picks ink off a print that was otherwise dry enough, and it will keep doing so on every job until it is cleaned.
Potential issues & solutions
When to escalate to technical support
Work the relevant section above first, as most defects resolve at press. Escalate when:
- the defect returns on the next job with a different design, ink and substrate combination
- corrective action on one variable produces a second defect elsewhere in the print
- adhesion or bond strength is involved and the product is destined for lamination, retort or food contact
- the fault appears across more than one press in the plant
Our technical support is here to help
DF Inks' technical service team works on site with converters across Europe, the Middle East and Africa, supported by our own laboratories and production facilities in Greece, Romania and Nigeria. We formulate the ink, so we can customize it for converters not just recommend a workaround.
FAQs about rotogravure printing defects
The most common causes are an ink chemistry that does not match the substrate, inadequate surface treatment, insufficient drying, and contamination on the film surface. Check the film's treatment level first, corona treatment decays during storage, and an aged film will fail a tape test regardless of ink performance.
Hazing is a fine ink mist left in the non printing areas, which also raises colour density in the unprinted areas. It means the doctor blade is not wiping the cylinder cleanly, through blade setting, blade parallelism, cylinder surface roughness or chrome quality, or because high ink viscosity is lifting the blade bevel.
Comets are short stripes that come and go at random, caused by debris or a nick passing under the blade. Hazing is a continuous mist across the non printing areas, caused by the blade failing to wipe the cylinder properly. Comets travel, hazing does not.
Many can be corrected in-run, particularly viscosity, doctor blade pressure, oven temperature and air velocity. Defects rooted in the cylinder, the chrome surface or the substrate batch require a stop. Change one variable at a time and record the result, simultaneous adjustments make the cause impossible to identify.